STANDARD TYPE
GRADE |
CHEMICAL COMPOSITION |
SPECIFIC GRAVITY
20°C g/ml |
VISCOSITY
20°C mPa.s |
GAP FILLING
microns |
SPEED OF BONDING |
TENSILE STRENGTH
DIN 53288
N/mm² |
SHEAR STRENGTH
DIN 53283
N/mm² |
IMPACT STRENGTH
ASTM D 950
N.mm/mm² |
23 |
ETHYL |
1,06 |
40 - 80 |
10 - 60 |
3 |
18 - 25 |
13 - 18 |
13 - 18 |
25 |
ETHYL |
1,07 |
300 - 500 |
10 - 150 |
2 |
18 - 23 |
13 - 18 |
15 - 20 |
32 |
ETHYL |
1,05 |
10 - 20 |
10 - 40 |
5 |
18 - 25 |
13 - 18 |
13 - 18 |
34 |
ETHYL |
1,06 |
30 - 60 |
10 - 100 |
5 |
18 - 25 |
13 - 18 |
13 - 18 |
43 |
ETHYL |
1,06 |
100 - 150 |
10 - 150 |
4 |
22 - 25 |
15 - 20 |
15 - 20 |
14 |
METHYL |
1,15 |
100 - 150 |
10 - 100 |
2 |
25 - 30 |
20 - 25 |
10 - 15 |
63 |
ALCOXY |
1,07 |
100 - 150 |
10 - 150 |
1 |
10 - 25 |
14 - 22 |
15 - 20 |
Relative setting time : 5 = highest speed, 1 = lowest speed.
SPECIALTY TYPE
GRADE |
CHEMICAL COMPOSITION |
SPECIFIC GRAVITY
20°C g/ml |
VISCOSITY
20°C mPa.s |
GAP FILLING
microns |
SPEED OF BONDING |
TENSILE STRENGTH
DIN 53288
N/mm² |
SHEAR STRENGTH
DIN 53283
N/mm² |
IMPACT STRENGTH
ASTM D 950
N.mm/mm² |
17 |
METHYL |
1,19 |
1100 - 1600 |
10 - 200 |
1 |
25 - 30 |
20 - 25 |
10 - 15 |
27 |
ETHYL |
1,08 |
1200 - 1800 |
10 - 200 |
2 |
18 - 25 |
13 - 18 |
13 - 18 |
29 |
ETHYL/BLACK |
1,08 |
1000 - 1500 |
10 - 200 |
1 |
18 - 25 |
13 - 18 |
13 - 18 |
41 |
ETHYL |
1,05 |
20 - 50 |
10 - 40 |
5 |
18 - 25 |
13 - 18 |
15 - 20 |
45 |
ETHYL |
1,08 |
800 - 1200 |
10 - 200 |
4 |
22 - 25 |
15 - 20 |
15 - 20 |
61 |
ALCOXY |
1,06 |
20 - 40 |
10 - 40 |
2 |
10 - 20 |
14 - 22 |
15 - 20 |
Relative setting time : 5 = highest speed, 1 = lowest speed.
PHYSICAL PROPERTIES
| FLASH POINT ISO 2592 ( °C ) |
87 |
| OPERATING TEMPERATURE ( °C ) |
-50 +80 |
| SOFTENING RANGE ( °C ) |
160/170 |
| REFRACTIVE INDEX n sup.20 sub.D |
SIMILAR TO GLASS |
| ELECTRICAL RESISTIVITY DIN 53482 ( OHM x mm ) |
>10 E 15 |
| DIELECTRIC STRENGTH DIN 53481 ( Kv/mm ) |
25 |
| DIELECTRIC CONSTANT DIN 53483 ( 1 MHz ) |
5,2 |
Information complémentaires : loxeal@sobelus.be
|